Galvanized Temporary Gates: What to Check on the Finish at Delivery
Agree which areas of a temporary gate will be inspected and how coating thickness and repairs will be documented. Pay particular attention to hinge brackets, latch posts and surfaces that rub during operation.

Why the Finish of a Gate Is Inspected Differently
A mobile access gate carries the same finishes as the fence beside it: galvanizing, or galvanizing with a powder coating. It differs in how the finish is stressed.
Thickness
Thickness is measured with a magnetic gauge, adjusted on uncoated material of the same form. On a duplex finish the zinc is measured before powder coating so that the two layers can be reported separately.
| Location | Reason |
|---|---|
| Hinge stile, front and back, at each hinge | Highest wear and load |
| Latch stile at the latch and at hand height | Handled at every operation |
| Wheel bracket and drop-bolt guide | Abrasion and ground contact |
| Inside corners and recesses | Faraday-cage areas |
Adhesion
Adhesion is checked by the cross-cut test (ISO 2409 or ASTM D3359) on flat test panels coated with each batch, and periodically on a leaf.
At edges and welds: a firm scrape with a blunt blade at a sharp edge and across a weld toe. Coating that flakes ahead of the blade will chip in service.
After forming or adjustment: if hinges or brackets are adjusted or straightened after coating, the bent area is examined for cracking and lifting.
Defects
| Defect | Consequence in a gate |
|---|---|
| Missed or incomplete weld | Joint has no strength; leaf racks |
| Undercut | Notch in the thin wall at the weld toe; fatigue crack start |
| Porosity | Reduced section; rust bleeding through coating |
| Crack | Grows in service; not acceptable at any size |
| Spatter and rough profile | Injury hazard; poor coating coverage |
Porosity
Porosity means discontinuities through the coating to the layer beneath: pinholes, craters, bare spots and cracks.
Visual Defects
| Zone | Surfaces |
|---|---|
| A | Public-facing faces of stiles and rails; hand-contact areas |
| B | Site-facing faces; mesh; infill |
| C | Undersides; inside of brackets; areas hidden in use |
| Defect | Cause |
|---|---|
| Bare spots; missed areas | Shielding; poor wetting; contact points |
| Sharp zinc spikes, drips; weld spatter under coating | Drainage; unprepared welds |
| Pinholes and craters | Outgassing |
| Jig marks | Hanging points |
| Scratches and chips from handling | After coating |
Visual inspection needs defined conditions, or it becomes a matter of opinion. Three things are fixed: the lighting, the viewing distance, and the classification of surfaces.
When Field Repair Is Needed
Galvanized coatings on temporary fencing, hoarding and barriers are damaged in three ways: by welding carried out after galvanizing, by mechanical damage in handling and use, and by cutting or drilling on site.
Acceptance Checks
| Check | Method |
|---|---|
| Coverage | Visual |
| Dry film thickness | Magnetic thickness gauge, after cure; at least three readings per repair on a sample of repairs |
| Adhesion | Firm scrape with a blunt knife at the edge of the repair; or cross-cut on test areas |
| Cure | Thumbnail or solvent rub as the data sheet describes |
| Appearance | Visual |
| Record | Repair log |
Surface Preparation
Preparation decides the life of the repair. Zinc-rich paint works only if its zinc particles are in electrical contact with bright steel; solder and sprayed zinc bond only to clean metal. The area prepared must extend into the sound galvanizing around the damage so that the repair overlaps it.
Remove contaminants first: oil, grease and soluble salts are washed off before mechanical cleaning, or they are spread and driven into the surface.
What to Expect of a Repair
It is softer, so it wears through at contact points; it is a paint, so it ages in sunlight; and its sacrificial action is weaker than that of solid zinc. Repairs should therefore be listed for inspection, and re-coated when they wear or when rust staining appears at their edges.
Sampling, Records and Release
Records: leaf serial or lot, coating batch, pretreatment and oven records, thickness readings with locations, adhesion and cure results, defects found and repairs made, inspector and date.
Every leaf: visual inspection of all zones; thickness at the hinge and latch stiles; touch-up of any defects found, with re-inspection.
Each coating batch: full thickness survey of one leaf; cross-cut on test panels; cure test as the powder supplier specifies.
Periodically: wet adhesion; porosity test on a leaf; comparison of colour and gloss with the retained reference.
Separate a transport scuff from a functional defect
A mark on a visible rail and a raised burr at the latch affect the gate differently. Record the location and whether the protection or movement is affected. Ask for the approved repair method, then inspect the finish and operate the gate again after the repair.
Frequently asked questions
What parts of a galvanized temporary gate should be checked on delivery?
Inspect welds, cut edges and visible coating damage. In a trial assembly, check hinges, latch and moving clearances against the agreed drawing.
How should a zinc burr near a latch be handled?
Record the location, affected lot and effect on operation. Hold the gate for an agreed repair or replacement and check the coating and latch again before acceptance.
Related product and planning information
Temporary fence gates · Quality control
Further reading
Browse articles
Temporary Fence Gates for Events: Pedestrian and Vehicle Access
List each opening by the people or vehicles that use it, how often it opens and the clear width it has to provide. A gate's quoted frame size can differ from the usable opening.

Galvanized Temporary Fence Panels: Pre-Galvanized or Hot-Dip After Fabrication?
The word “galvanized” can describe different production routes. Confirm whether zinc was applied to the strip before forming or to the finished assembly, and ask how seams, cut edges and welds are protected.

Bulk Temporary Fence Panels: What to Inspect Before Accepting a Shipment
Set acceptance checks before the order goes out. On delivery, use the approved drawing to identify misalignment, damaged joints, bowing and sharp edges, and record the lot before any affected stock is released.